Posted by Denis 
Drops (snot) printing
August 30, 2011 04:09PM
Who have experienced this and how to solve?
When printing on the edges remain snot.
I publish a RepRap Host.
Time Extruder_Reverse - 2300 ms.
Heat at 260 degrees (ABS).
Attachments:
open | download - mesh.JPG (62.8 KB)
Re: Drops (snot) printing
August 30, 2011 04:34PM
Too much heat? ABS too runny..?
Re: Drops (snot) printing
August 30, 2011 04:41PM
I dont know.
You think need lower heat?
I try.
VDX
Re: Drops (snot) printing
August 30, 2011 05:18PM
... i'm printing with PLA in sprinter/printrun and had the same blobs when my extra distance after retract was set to big.

With proper adjustment (last settings: retract =5mm, extra distance =2mm) i eliminiated the blobs, but this is highly depending on nozzle diameter, printing speed (or applied pressure) and viscosity of the material.

Actually i've tightened the nozzle diameter and changed the material, so i have to adjust the parameters anew ... in the last print i had some 'blobbing' again, but not clearly defined, so ia have to adjust the printing speed in order to get better results.


Viktor
--------
Aufruf zum Projekt "Müll-freie Meere" - [reprap.org] -- Deutsche Facebook-Gruppe - [www.facebook.com]

Call for the project "garbage-free seas" - [reprap.org]
Sorry, only registered users may post in this forum.

Click here to login